关于ZnO/Si(100)接口的SIMS特性的一个简短说明
A short note on the SIMS characterisation of ZnO/Si(100) interface
摘要:
通过电子束蒸发将ZnO(99.9%)颗粒沉积到自然氧化物覆盖的硅(100)衬底上,沉积25 nm厚的ZnO膜。详细的界面化学组成和化学深度分布如下:吸附OH表面/OH:ZnO界面/纯ZnO薄膜/ZnO:H:Si界面/H:SiO2/SiO2/Si(100)。通过SIMS深度轮廓形成的凹坑的物理轮廓用P2P或P-2轮廓仪测量,因为深度轮廓显示出均匀的离子研磨和与通过SIMS深度轮廓(25.4nm)测量的膜厚度(25 nm)的良好一致性。
英文摘要:
The ZnO films, 25 nm thick were deposited by e-beam evaporation of ZnO (99.9%) pellets onto native oxide covered silicon (100) substrates. Details of the interface chemical composition and the chemical depth profile have been deduced as follows: Adsorbed OH surface/OH: ZnO Interface/Pure ZnO thin film/ZnO:H: Si Interface/H:SiO2/SiO2/Si(100). The physical profile of the crater formed by the SIMS depth profiling was measured with a Tencor P-2 profilometer as depth profiling showed uniform ion milling and good consistency with film thickness (25 nm) measured by SIMS depth profile (25.4 nm).