湿度对金薄膜纳米结构的影响

Moisture Effects on Nanowear of Gold Films

Xiaolu Pang, Alex A. Volinsky, Kewei Gao

摘要:

利用扫描纳米压痕仪研究了溅射Au薄膜在干、湿环境中的纳米磨损特性。在10 microN的相同正常载荷下,与空气相比,金在水中的磨损率高出10倍以上。从划痕试验中获得的摩擦系数保持恒定在0.2,无论测试条件如何。金表面粗糙度增加3至8纳米后,在空气中200磨损循环。在水中经过200次磨损循环后,在Au膜表面上产生了200 nm高的表面波纹。薄膜的划痕硬度与纳米压痕硬度相当。

英文摘要:

Nanowear properties of sputtered Au films in dry and wet environments were investigated using a scanning nanoindenter. Gold exhibits over 10 times higher wear rate in water compared to air at the same normal load of 10 microN. The friction coefficient obtained from scratch tests remained constant at 0.2 regardless of the testing conditions. Au surface roughness increased from 3 to 8 nm after 200 wear cycles in air. Surface ripples, 200 nm high developed on the Au film surface after 200 wear cycles in water. Film scratch hardness compares well with the nanoindentation hardness.

机构、总结、中文摘要均由AI分析而来,可能存在错误,请以论文正文为准。

↑